Gland packing and rubber sheet for pumps, valves and gaskets
Compression packing for pump and valve stuffing boxes, low-emission valve packing sets, and rubber and fiber sheet for gaskets, linings and pads. Sourced from established makers and supplied from Al Jubail with the maker’s data sheets.
Gland packing and rubber sheet are the two everyday sealing consumables of a plant: braided rings that seal a moving shaft or stem, and elastomer sheet from which flat gaskets, linings and pads are cut. Gland (compression) packing is pressed into a stuffing box around a pump shaft or valve stem. Choose it by temperature, pH, pressure and shaft speed: PTFE for chemicals, graphite for heat and steam, aramid for abrasives. Rubber sheet is chosen by fluid and temperature: NBR for oil, EPDM for water and weather, neoprene for general outdoor use, FKM (fluoroelastomer) for hot oils and chemicals.
- Packing types
- Braided PTFE, ePTFE with graphite, flexible graphite with nickel-alloy wire, aramid, carbon fiber, die-formed graphite rings
- Packing sizes
- Square sections typically 3 to 25 mm (1/8 to 1 in.); die-formed rings to the box size
- Packing forms
- Spools or coils by weight, pre-cut ring sets, valve packing sets with end rings
- Valve emissions
- Packing type-tested to API 622 where your valve specification calls for it, with the maker’s report
- Rubber sheet
- NBR, EPDM, neoprene (CR), FKM (fluoroelastomer), natural rubber, silicone, SBR, cloth-insertion sheet
- Sheet sizes
- Typically 1.5 to 25 mm thick; rolls about 1.2 to 1.4 m wide and about 10 m long
- Hardness
- Commonly 60 to 70 Shore A, tolerance about plus or minus 5 (tested to ASTM D2240)
- Fiber sheet
- Compressed non-asbestos fiber sheet (aramid and inorganic fibers with NBR binder)

What we supply
- Pump packing
- Braided PTFE, ePTFE with graphite, aramid and carbon fiber in coils or cut ring sets
- Valve packing
- Flexible graphite with nickel-alloy wire, braided PTFE and low-emission sets
- Die-formed rings
- Graphite rings pressed to the stem and box size, with braided end rings
- Rubber sheet
- NBR, EPDM, neoprene, FKM, natural rubber and silicone by the roll or cut length
- Insertion rubber
- Rubber sheet with one or more plies of cloth for water and pump flanges
- Fiber sheet
- Compressed non-asbestos sheet for general-service flat gaskets
Gland packing types compared
Each packing type has a working window of temperature, pH, pressure and shaft speed. The figures below are typical values from published maker data sheets; they vary by maker and style, so confirm against the data sheet of the exact style you buy.
| Packing type | Typical temperature | Typical pH | Typical pressure | Typical shaft speed | Best for |
|---|---|---|---|---|---|
| Braided PTFE | -200 to +280 °C | 0 to 14 | About 20 bar rotary, 200 bar valves | About 10 m/s | Chemical pumps and valves, clean and food service |
| ePTFE with graphite | -240 to +288 °C | 0 to 14, except strong oxidizers | About 20 bar (300 psi) in pumps | About 20 m/s | General-service and high-speed pumps, mixers, agitators |
| Flexible graphite with nickel-alloy wire | -240 to 450 °C in air; 650 °C in steam | 0 to 14, except strong oxidizers | 400 to 580 bar static, by maker | Valve service (about 1 m/s) | High-pressure steam and hot hydrocarbon valves |
| Aramid | About -100 to +260 °C | About 2 to 12 (some styles 1 to 13) | About 20 to 34 bar in pumps | About 9 to 25 m/s by style | Abrasive slurries, paper stock, wastewater |
| Carbon fiber | Up to about 280 to 288 °C | About 1 to 14 or 2 to 12, by style | About 30 to 35 bar in pumps | About 15 m/s | Hot water, chemicals, pumps and agitators |
| Die-formed graphite rings | -200 to about 450 to 500 °C in air; 650 °C in steam | 0 to 14 | Up to about 250 bar on valve stems (one maker) | Mainly valve stems | Valve stem sets with braided end rings |
Typical values only, taken from published maker data sheets; limits differ between makers and styles, and the maximums for temperature, pressure and speed are not meant to be reached together. Strong oxidizers such as fuming nitric acid and oleum attack graphite and many lubricants.
Rubber sheet compounds compared
Choose rubber sheet by the fluid first and the temperature second. Temperatures below are typical continuous ranges published by sheet suppliers; grades differ, so check the maker’s sheet for the compound you buy.
| Compound | Typical temperature | Resists | Avoid | Typical uses |
|---|---|---|---|---|
| NBR (nitrile) | -40 to +100 °C | Oils, fuels, hydraulic fluids | Hot water above about 70 °C, steam, ketones, aromatics, outdoor ozone | Oil-service gaskets, pads and linings |
| EPDM | -50 to about +120 to 150 °C | Water, low-pressure steam, ozone, UV, dilute acids and alkalis | Petroleum oils, fuels, solvents | Water and cooling-water flanges, outdoor seals |
| Neoprene (CR) | -40 to +100 °C | Weather, ozone, seawater, moderate oils | Strong oxidizing acids, aromatic or chlorinated solvents, ketones | Marine and HVAC gaskets, general pads |
| FKM (fluoroelastomer) | -20 to +200 °C (some grades 250 °C) | Hot oils, fuels, many chemicals | Use where NBR or EPDM will do; it costs several times more | Hot oil and chemical service gaskets |
| Natural rubber (NR) | About -50 to +70 °C | Abrasion, tear, water | Oil, ozone, weathering, heat above 70 °C | Chute and hopper lining, wear and damping pads |
| Silicone (VMQ) | -60 to +230 °C | Heat and cold, food-grade options | Petroleum oil, high-pressure steam, tearing and abrasion | Oven and hot-air seals, food and electrical use |
| SBR and cloth-insertion sheet | About -30 to +80 °C | Water and air; cloth plies add tear strength | Oil, ozone, hot water | Water main and pump flange gaskets, general pads |
| Compressed non-asbestos fiber | About 220 °C continuous (one maker) | Oils, gases, light chemicals | Use above the maker’s pressure-temperature limit | General-service flat gaskets |
Typical values from supplier data; the compound, hardness and grade of each maker differ. Rubber compounds are classified under ASTM D2000; nonmetallic fiber gasket materials under ASTM F104.
Gland packing and rubber sheet in Saudi plants
Eastern Province plants put packing and rubber through heat, sun, chlorides, sand and sour hydrocarbons. The points below are what to check; your project specification and valve data sheets are the final word.
| Requirement | What it means |
|---|---|
| Import conformity | Products under a SASO technical regulation are registered on the SABER platform, which issues product and shipment conformity certificates. |
| No asbestos | Saudi Arabia is on the international list of national asbestos bans. Specify non-asbestos packing and sheet, and keep the maker’s statement on file. |
| Heat, sun and ozone | Outdoor rubber ages fast. EPDM and neoprene resist ozone and UV better than NBR or natural rubber; store rolls out of direct sun. |
| Seawater and sand | Seawater intake and cooling pumps at Jubail Industrial City and Ras Al Khair carry chlorides and fine sand. Use abrasion-tolerant packing, a clean flush and hardened sleeves. |
| Sour and hydrocarbon valves | Valve packing in hydrocarbon service is often graphite with a corrosion inhibitor. API 622 includes corrosion and material requirements for packing. |
| Fugitive emissions | If the valve specification calls for API 622, API 624 or ISO 15848-1, ask for the test report that covers the exact packing style and size range. |
We have not cited any Saudi Aramco or SABIC document for this product. Check the packing, gasket and elastomer requirements in your project specification, line class and valve data sheets before ordering.
Where gland packing and rubber sheet are used
Packing seals moving shafts and stems; sheet becomes flat gaskets, linings and pads.
Centrifugal and reciprocating pumps
Cooling water, seawater, slurry, chemical and condensate pumps with packed stuffing boxes.
Valve stems
Gate, globe and plug valves in steam, water and hydrocarbon service, including low-emission sets.
Mixers and agitators
Slow and medium speed shafts on tanks, where ePTFE with graphite or aramid is common.
Flat gaskets from sheet
Rubber and fiber sheet cut by your maintenance team or gasket cutter for flanges, manholes and covers.
Linings and pads
Natural rubber and SBR for chutes and hoppers; neoprene and NBR for bearing, anti-vibration and machine pads.
Shutdown stores
Packing coils, ring sets and sheet rolls listed per pump or valve tag for turnaround work.
Sourced from established makers
We supply packing and sheet; we do not manufacture or cut them. Each item comes in the maker’s packaging with its style, size and batch shown.
- Maker’s data sheet
- Style and size on every coil
- Pre-cut ring sets where the maker offers them
- Sheet by roll or cut length
- Matched to your pump and valve list
Documents and inspection
Ask for the documents your specification needs when you send the enquiry, so we source the right lot.
- ISO 9001 quality system
- API 622 test report where specified
- Non-asbestos statement
- Third-party inspection on request
What gland packing is and how it seals
Gland packing is a set of braided rings pressed into a stuffing box around a shaft or stem. A gland follower, pulled down by two or more studs, squeezes the rings so they press against the shaft and the box bore. That radial pressure is what seals.
Pump packing and valve packing work differently. Pump packing is meant to leak a small, steady amount, because the leakage lubricates and cools the packing against a shaft turning at speed. Valve packing is meant to show no visible leakage, because the stem moves slowly and only now and then.
Many pump stuffing boxes also hold a lantern ring. This is a spacer ring with holes, placed in line with a port in the box, through which clean water or another flush is fed. The flush cools the rings and keeps abrasive solids away from the shaft.
Packing or mechanical seal?
Mechanical seals have replaced packing on many process pumps, but packing remains common on water, seawater, slurry and utility pumps and on almost every rising-stem valve. It is cheap, it can be replaced without taking the pump apart, and it tolerates shaft movement that would damage a seal face.
The trade-off is leakage and maintenance. A packed pump needs a drain for the leakage, regular gland checks and, every so often, a full repack.
Gland packing types and what each one does
Packing is named after its yarn: the fiber that is braided into a square section. The yarn decides the temperature, chemical and speed limits. The braid and the lubricant decide how well the packing conforms and how fast it beds in.
Braided PTFE
PTFE yarn packing is chemically inert across pH 0 to 14 and typically runs from -200 to about +280 °C. It suits chemical pumps and valves and clean services. Its weakness is heat: PTFE conducts heat poorly, so typical shaft speeds are about 10 m/s.
Expanded PTFE with graphite
Expanded PTFE yarn loaded with graphite carries heat away from the shaft much better than plain PTFE. Published data for these styles give about -240 to +288 °C, pH 0 to 14 except strong oxidizers, and shaft speeds of about 20 m/s. It is a common general-service pump packing because one style covers most fluids in a plant.
Flexible graphite with nickel-alloy wire
Flexible graphite yarn reinforced with nickel-alloy wire is a standard valve packing for steam and hot hydrocarbons. Published limits are about 650 °C in steam and about 450 °C in air, with static pressures of 400 to 580 bar depending on the maker. The wire stops the soft graphite from extruding past the gland and stem.
Aramid
Aramid fiber is very strong and resists abrasion, so it is used for slurries, paper stock, fly ash and wastewater. Typical limits are about -100 to +260 °C and a narrower pH band of about 2 to 12. Because aramid is hard, makers recommend hardened shafts or sleeves and a flush to avoid scoring.
Carbon fiber
Carbon fiber packing handles heat and most chemicals and conducts heat well. Lubricated styles are typically rated to about 280 to 288 °C and about 15 m/s. It is used in hot water, chemical and pulp-and-paper pumps, mixers and agitators.
Die-formed graphite rings
Die-formed rings are pressed from expanded graphite foil into solid rings of a set density, often about 1.5 to 1.6 g/cm3. They seal valve stems at up to about 650 °C in steam and about 450 to 500 °C in air, depending on the maker. They are usually installed as a set, with braided end rings above and below to stop the soft rings extruding.
How to choose gland packing and rubber sheet
Start with the fluid, then the temperature, then the pressure, then the shaft speed. A packing that passes all four limits with margin is a candidate; pick the one with the best record in that service in your plant.
For rubber sheet the order is the same: fluid first, then temperature, then pressure, then the mechanical duty such as abrasion or compression set. Choosing the wrong compound for the fluid causes most rubber gasket failures.
- Check that temperature, pressure and speed are each within the data sheet, not just one of them.
- Check the pH range and the exclusions, such as strong oxidizers for graphite.
- For pumps, check the shaft or sleeve hardness and condition; hard packings need hard sleeves.
- For valves, check whether the specification calls for API 622 tested packing or a fire-tested set.
- For sheet, check outdoor exposure; sun and ozone crack NBR and natural rubber.
| Service | Pump packing | Valve packing | Sheet |
|---|---|---|---|
| Cooling water and seawater | ePTFE with graphite, or aramid where sand is present | Braided PTFE or graphite | EPDM, neoprene or cloth-insertion rubber |
| Steam and boiler feed | Carbon fiber or graphite styles rated for the temperature | Flexible graphite with nickel-alloy wire, or die-formed set | Compressed fiber sheet within its limits; spiral wound above |
| Hydrocarbons and oils | ePTFE with graphite or carbon fiber | Graphite set, API 622 tested where specified | NBR, or FKM for hot oil |
| Acids and alkalis | PTFE or ePTFE with graphite | PTFE or graphite with inhibitor | EPDM for dilute acids and alkalis; check charts |
| Slurries and abrasives | Aramid with flush and hardened sleeve | Not usually packed valves; check the valve maker | Natural rubber or SBR for linings |
| Food and potable water | PTFE or ePTFE with suitable approvals | PTFE | EPDM or silicone with suitable approvals |
How to measure the stuffing box and order the right size
The packing cross-section is half the difference between the stuffing box bore and the shaft or sleeve diameter. The number of rings is the box depth divided by that cross-section, rounded to the nearest whole ring. Measure on the equipment, not from an old ring, because used packing is crushed and worn.
Worked example
A pump has a 55 mm sleeve, a 75 mm box bore and a 52 mm deep box. The cross-section is (75 – 55) / 2 = 10 mm. The ring count is 52 / 10 = 5.2, so 5 rings of 10 mm packing.
In inches: a 2 in. sleeve in a 3 in. bore gives (3 – 2) / 2 = 1/2 in. packing. A 2 1/2 in. deep box then takes 5 rings.
One maker advises no more than five to seven rings; in deeper boxes a bushing is fitted at the bottom so a shorter set can be used.
Standard sizes
Square packing is commonly made from about 3 mm (1/8 in.) to 25 mm (1 in.). One maker’s range runs in 1/16 in. steps from 1/8 to 5/8 in., then 3/4, 7/8 and 1 in. Die-formed graphite rings are made to the stem and box diameters, with sections from about 1.5 mm upward.
- Measure the shaft or sleeve diameter where the packing runs (call it d).
- Measure the stuffing box bore (call it D).
- Measure the box depth from the bottom of the box to the face where the gland starts.
- Cross-section = (D minus d) divided by 2. Round to the nearest standard size.
- Number of rings = depth divided by cross-section, rounded to the nearest whole number.
- If a lantern ring is fitted, take away one or two rings depending on the lantern ring’s height.
- Record the gland stud size and number of studs, so the gland can be tightened evenly.
Cutting rings and installing pump packing
Cut each ring separately on a mandrel the same diameter as the shaft or sleeve, and check its fit before you install it. Never wind a continuous coil into the box; it cannot be compressed evenly and leaks along the spiral.
Butt cut or skive cut
A butt cut is straight across, so the two ends meet squarely. It is used mostly on rotating equipment. A skive cut is at 45 degrees, so the ends overlap; it is used mostly on valves. Some makers prefer a 45 degree cut for pumps too, so follow the packing maker’s instruction.
Cut cleanly with a sharp knife or packing cutter. Ragged ends leave a leak path and fray in service.
Installing the rings
Isolate the pump, drain it and release the pressure. Remove every old ring and the lantern ring with a packing hook; do not use system pressure to blow them out. Inspect the shaft or sleeve for nicks and scoring and replace it if needed.
- Fit each ring on its own and seat it firmly to the bottom of the box with a split bushing or the gland.
- Stagger the joints: 180 degrees apart for two rings, 120 degrees for three, 90 degrees for four or more.
- If a lantern ring is used, line it up with the flush port.
- Leave the gland entered at least about 3 mm (1/8 in.) into the box, with room for later adjustment.
- Turn the shaft by hand to check it does not bind.
Run-in and leakage
Start the pump with the gland nuts only finger tight and allow generous leakage. Then tighten the nuts slowly and evenly, about one flat at a time, until the leakage settles at the level the packing maker gives.
Leakage figures vary by style. One maker gives 1 to 5 drops per minute per inch of shaft diameter for a carbon-graphite style. New packing can run warm, or steam slightly, during the first hours of break-in.
Do not try to stop all leakage on a pump. A dry packing overheats, hardens and scores the sleeve. Repack when the leakage can no longer be controlled or the gland has no travel left.
Low-emission valve packing: API 622, API 624 and ISO 15848-1
Low-emission valve packing is packing type-tested to show very low methane leakage at the stem over many thermal and mechanical cycles. It is required where a project limits fugitive emissions of hydrocarbons and volatile organic compounds.
API 622 tests the packing alone in a standard fixture. API 624 then tests a complete rising-stem valve, and it requires that the packing has already passed API 622. That is the link between the two: API 622 qualifies the packing; API 624 qualifies the valve built with it.
What to ask for
Ask for the API 622 test report of the exact packing style, and check that the size range covers your stems. The third edition added a 1/8 in. sample test to the original 1/4 in. test. If the valve itself must meet API 624 or ISO 15848-1, that is the valve maker’s qualification, not the packing supplier’s.
Low-emission sets are often die-formed graphite rings with braided end rings, sometimes live-loaded with disc springs on the gland studs to keep the load on as the packing relaxes.
| Standard | What is tested | Key test figures (as published) |
|---|---|---|
| API 622 (Type Testing of Process Valve Packing for Fugitive Emissions) | The packing set in a standard test fixture | Methane at 600 psig, ambient and 500 °F, 1,510 mechanical cycles, 5 thermal cycles; third edition leak limit 100 ppmv with no gland adjustment; also corrosion and material requirements |
| API 624 (Type Testing of Rising Stem Valves Equipped with Graphite Packing for Fugitive Emissions) | A complete rising or rising-rotating stem valve with API 622 packing | 310 mechanical cycles, 3 thermal cycles, 100 ppmv leak limit; the 2023 second edition excludes valves above NPS 42 or above Class 1500 (the 2014 first edition stopped at NPS 24) |
| API 641 | Quarter-turn valves | 610 cycles, 100 ppmv; graphite packing must first pass API 622 |
| ISO 15848-1 | Type testing of industrial valves for fugitive emissions | Tightness classes with helium (AH, BH, CH) or methane (AM, BM, CM), plus endurance and temperature classes |
Rubber sheet: compounds, hardness, thickness and rolls
Rubber sheet is calendered elastomer sold in rolls or cut lengths. Plants cut it into flat gaskets for low-pressure flanges, manholes and covers, and use it for linings, wear strips, pads and anti-vibration mounts.
The compound sets the fluid and temperature limits. The hardness sets how well it seals and how much it creeps. Hardness is measured in Shore A with a durometer to ASTM D2240; most gasket sheet is 60 to 70 Shore A with a tolerance of about plus or minus 5.
Thickness and roll sizes
Common thicknesses run from about 1.5 to 25 mm. Thin sheet of 1.5 to 3 mm is used for gaskets; 4 to 6 mm for general sealing and damping; 10 mm and above for heavy pads and isolation.
Rolls are typically about 1.2 or 1.4 m wide and about 10 m long, with a width tolerance of a few percent. Inch-based cloth-insertion sheet is often 48 in. wide in rolls of 18 to 67 ft.
Cloth-insertion rubber
Insertion rubber has one to four plies of cotton, nylon or polyester fabric inside the sheet. The fabric raises tear strength and stops the rubber flowing out under bolt load. One supplier gives about 25 bar for insertion sheet against about 10 bar for plain sheet.
It is the usual choice for water main and pump flange gaskets. It is not suitable for oil unless the base compound is NBR or neoprene.
Gaskets cut from sheet
We supply the sheet; your maintenance team or a specialist gasket cutter cuts the gaskets. For flange gaskets, one supplier recommends about 70 Shore A EPDM at 2 to 3 mm: softer sheet bulges under bolt load and harder sheet does not conform to the flange face.
Above the limits of rubber, move to compressed fiber, PTFE or a spiral wound gasket.
Compressed non-asbestos fiber sheet and other alternatives
Compressed non-asbestos fiber sheet (often called CNAF) is a better gasket sheet than rubber where heat, pressure or hydrocarbons rule rubber out. It is made from aramid and inorganic fibers bound with NBR, and sometimes with neoprene or EPDM.
One maker lists about 220 °C (430 °F) continuous and 380 °C (720 °F) intermittent for a general-purpose grade, with a pressure-temperature limit that falls as temperature rises. The same maker notes that thinner sheet performs better at high temperature under pressure.
Classification
Fiber gasket sheet is described with the ASTM F104 classification system for nonmetallic gasket materials, as a line callout made of a type number and property codes. Rubber compounds are not in F104; they are classified under ASTM D2000.
When to step up
Move from sheet to a semi-metallic gasket when the flange class, temperature or fluid exceeds the sheet maker’s limits. Spiral wound gaskets suit most Class 150 to 2500 process flanges; ring type joints suit high-pressure Class 600 and above where the flanges are grooved.
| Option | Strength | Limit |
|---|---|---|
| Gland packing | Cheap, repairable in place, tolerant of shaft movement | Needs leakage on pumps and regular adjustment |
| Mechanical seal | Near-zero leakage on pumps | Higher cost; needs a clean, stable shaft |
| Rubber sheet gasket | Seals at low bolt load; easy to cut | Low temperature and pressure limits |
| Compressed fiber gasket | Higher temperature and pressure than rubber | Limited by pressure-temperature factor |
| Spiral wound gasket | Process flanges at high temperature and pressure | Needs correct bolt load and flange finish |
How to specify gland packing and rubber sheet on an RFQ
A clear enquiry names the service, the size and the documents. With that, we can source the right style first time instead of trading emails.
For gland packing
- Equipment and tag: pump, valve, mixer or agitator, with the tag number if you have one.
- Service: fluid, temperature, pressure, and shaft speed in rpm with the shaft diameter.
- Size: cross-section, or the box bore, shaft diameter and depth.
- Form: coil by weight or length, or pre-cut ring sets with the ring count.
- Packing type or the data sheet style you use now, and any approved equivalent.
- Documents: data sheet, API 622 report, non-asbestos statement, inspection needs.
For rubber and fiber sheet
- Compound: NBR, EPDM, neoprene, FKM, natural rubber, silicone, SBR or fiber sheet.
- Hardness in Shore A and the tolerance you accept.
- Thickness, width and length, or full rolls.
- Insertion plies, if any, and color if it matters for identification.
- Fluid and temperature, so the compound can be checked.
- Any food, potable water or other approval the service needs.
Example lines
ePTFE with graphite packing, 10 mm square, 5 kg coil, for seawater cooling pumps, 55 mm sleeves, 1,480 rpm.
Flexible graphite packing with nickel-alloy wire, 1/4 in., API 622 test report required, for steam gate valves to 400 °C.
EPDM rubber sheet, 3 mm thick, 70 Shore A plus or minus 5, 1.2 m x 10 m roll, quantity 4 rolls.
Inspection, storage and common mistakes
Check packing and sheet on receipt against the order, then store them so they arrive at the job in the same condition. Most packing and gasket failures trace back to the wrong material, the wrong size or poor installation, not to the product itself.
Receiving checks
- Style, size and batch on the label match the order and the data sheet.
- Packing is evenly braided, with no loose yarn, dry patches or damage to the coil.
- Die-formed rings are whole, of the right inside and outside diameter, with no cracks.
- Sheet thickness is within tolerance at several points across the width.
- Hardness is checked with a Shore A durometer if the order sets a value.
- Test reports and statements asked for in the order are present.
Storage
Keep packing in its packaging, clean and dry, away from grit. Store rubber sheet rolled or flat, in a cool place out of direct sun, because heat, UV and ozone crack many compounds. Use older stock first.
Common mistakes
- Using one cross-section for every pump instead of measuring each box.
- Winding a coil into the box instead of cutting separate rings.
- Lining up the ring joints, which gives a straight leak path.
- Tightening a pump gland until it stops leaking, which burns the packing.
- Using NBR sheet outdoors or in hot water, or EPDM in oil.
- Ordering valve packing for an emission-controlled valve without asking for the API 622 report.
Gland packing and rubber sheet questions
What is gland packing?
Gland packing, also called compression packing, is a braided rope of PTFE, graphite, aramid, carbon or other fiber that is cut into rings and pressed into a stuffing box around a pump shaft or valve stem. A gland follower squeezes the rings so they seal against the shaft and the box bore. Pumps allow a small leakage to cool the packing; valves should show no visible leakage.
How do I work out the packing size?
Measure the stuffing box bore and the shaft or sleeve diameter. The cross-section is the bore minus the shaft diameter, divided by two. For example, a 75 mm bore and a 55 mm sleeve give 10 mm packing. Then divide the box depth by the cross-section to get the number of rings, rounding to the nearest whole ring, and allow for a lantern ring if one is fitted.
What is the difference between a butt cut and a skive cut?
A butt cut goes straight across the packing, so the two ends meet squarely; it is used mostly on rotating equipment such as pumps. A skive cut is made at 45 degrees, so the ends overlap; it is used mostly on valves. Cut each ring on a mandrel the same size as the shaft, and follow the packing maker’s preference where it gives one.
How should packing joints be staggered?
Offset each ring joint from the one before so there is no straight leak path. A common rule is 180 degrees apart for two rings, 120 degrees for three rings and 90 degrees for four or more. Seat each ring on its own to the bottom of the box before fitting the next. Some valve packing instructions give a different stagger, so check the maker’s sheet.
How much should a packed pump leak?
It depends on the packing style, shaft size and speed, so use the packing maker’s figure. As an example, one maker gives 1 to 5 drops per minute per inch of shaft diameter for a carbon-graphite style. Start with generous leakage and tighten the gland nuts slowly and evenly. Never tighten until the leakage stops; the packing will overheat and score the sleeve.
Which packing is best for steam valves?
Flexible graphite packing reinforced with nickel-alloy wire, or a set of die-formed graphite rings with braided end rings, is the usual choice. Published limits are about 650 °C in steam and about 450 °C in air, depending on the maker. Where fugitive emissions are controlled, ask for packing that is type-tested to API 622 and check the report covers your stem size.
What is the relation between API 622 and API 624?
API 622 type-tests valve stem packing on its own in a standard fixture, using methane, thermal cycles and mechanical cycles. API 624 type-tests a complete rising-stem valve fitted with graphite packing, and it requires that packing to have passed API 622 first. So API 622 qualifies the packing and API 624 qualifies the valve. Both use a 100 ppmv leak limit in their current editions.
Can the same packing be used in pumps and valves?
Sometimes. Some styles, such as many PTFE and ePTFE with graphite packings, are rated for both. But pump packing is designed to run with controlled leakage at speed, while valve packing must seal with no visible leakage and often high pressure. Check that the data sheet lists the service, and use a valve-rated graphite packing for high-pressure steam and hydrocarbon valves.
Why do aramid packings need a hard sleeve?
Aramid fiber is strong and abrasion-resistant, which is why it suits slurries, paper stock and wastewater. The same hardness can wear a soft shaft or sleeve. Makers recommend hardened shafts or sleeves and a clean flush through the lantern ring to keep solids out and reduce scoring. Check the sleeve before repacking and replace it if it is grooved.
Which rubber sheet should I use for oil, water or outdoor service?
Use NBR (nitrile) for oils and fuels, EPDM for water, low-pressure steam and outdoor weathering, and neoprene for general outdoor, marine and moderate oil service. Use FKM (fluoroelastomer) for hot oils and aggressive chemicals, and silicone for high and low temperatures without oil. Do not use EPDM in oil or NBR in hot water or direct sun.
What hardness of rubber sheet is used for gaskets?
Most gasket sheet is 60 to 70 Shore A, with a tolerance of about plus or minus 5, measured with a durometer to ASTM D2240. One supplier recommends about 70 Shore A for EPDM flange gaskets, because softer sheet bulges under bolt load and harder sheet does not conform to the flange face. State the hardness and tolerance on the order.
What is insertion rubber sheet?
Insertion rubber is rubber sheet with one or more plies of cotton, nylon or polyester cloth built in. The cloth adds tear strength and stops the rubber flowing out under bolt load, so it holds higher pressure than plain sheet. It is common for water main and pump flange gaskets. The base compound, often SBR, NBR or neoprene, decides the fluid resistance.
When should I use compressed fiber sheet instead of rubber?
Use compressed non-asbestos fiber sheet when the temperature, pressure or hydrocarbon content is beyond rubber. It is made from aramid and inorganic fibers bound with NBR. One maker lists about 220 °C continuous for a general-purpose grade, with the pressure limit falling as temperature rises. Above its limits, use a spiral wound or other semi-metallic gasket.
Does JTE cut gaskets or make packing?
No. We supply gland packing, rubber sheet and fiber sheet sourced from established makers, in the maker’s packaging with its data sheet. Gaskets are cut from the sheet by your maintenance team or a specialist gasket cutter. Our factory in Al-Jubail cuts, threads and bends fasteners, such as the gland studs on your pumps and valves.
Updated
Related
Gaskets and rings
Spiral wound, ring type joint and sheet gaskets for process flanges.
Spiral wound gaskets
The step up from sheet gaskets for higher temperatures and pressures.
Industrial valves
Gate, globe, ball and check valves whose stems take this packing.
Send your packing and sheet list